Dear Lana,
Thanks so much for providing all of the information about this canoe. What a great object! (I love dugout canoes.) According to my notes, this is what we have established thus far:
- a dugout canoe made of tulip poplar (hardwood/angiosperm) was discovered and excavated in Nov. 1964
- a PEG treatment (molecular weight and concentration unknown) was attempted shortly thereafter: possible full immersion in PEG (assuming an unheated treatment) for ~2 days before receptacle failure, then ~2 months of "daily sprinkling with remaining solution," then returned to the Conner Prairie Museum in Sept. 1965 for exhibition
- the canoe now sits on a custom-made cradle made of stained and sealed poplar which doubles as its exhibition mount. Mount is a nearly 23' long, 4"x4" beam with supportive buttresses. The mount and canoe currently sit on the floor in collection storage which is a climate-controlled and stable environment
- the canoe weighs approximately 1900 lbs and takes ~12 ppl to lift/move it
- no major/active condition issues noted (in terms of wood cracking/flaking/splintering, discoloration, bio growth, gooey surfaces, pest activity, dust/grime accumulation on surface) other than the wood structure is spongy or punky in a few areas, and a few detached pieces which were knocked off during a move in the late 80s, which have been salvaged and kept in the collection
- possible exhibition in the distant future
- the last time it was moved was in 1998
My recommendation is to bring in an objects conservator https://www.culturalheritage.org/membership/find-a-conservator to do a thorough condition assessment and to execute high-resolution photographic documentation of the canoe. There may well be justification for conservation treatment, but I would entrust the conservator to make the best possible decisions about treatment materials and adhesives, if warranted. The assessment would also provide you with a time and cost estimate so that you can be prepared to implement the treatment when you are ready.
Here are some initial thoughts I have about the initial PEG treatment as well as recommendations for the future.
Given the object's size and weight and short duration of immersion and the unknown thoroughness of "daily sprinkling," I suspect that the PEG treatment only partially impregnated the wood structure (it is nearly impossible to confirm this without examining the canoe in person). Successful PEG treatments are dependent on adequate time, temperature, concentration, and wood quality/condition, amongst other factors. On the other hand, if the canoe managed to be dried without serious losses though, then the PEG may have performed adequately. All of which is to say, there are a lot of variables and unknowns here about the parameters of the original treatment.
In the interim, I recommend keeping the surface dust-free and fabricating a Tyvek dust cover to drape over the canoe while in storage awaiting treatment or exhibition. Also monitor the canoe periodically for any pest activity or bio growth, or any changes to the surface. I have reached out to a few experts in the field and am awaiting their responses. I'll update this post as I receive additional input for your case.
If you have any additional questions or comments, we are standing by!
Best,
------------------------------
Nicole Peters
Conservator
Peters Art Conservation Services, LLC
Skagway, AK 99840
------------------------------